**Author:** ![davidE1A](https://avatars.discourse-cdn.com/v4/letter/d/b19c9b/32.png) [@davidE1A](https://forum.snapmaker.com/u/davidE1A)\
**Post date:** [September 23, 2023, 4:54pm UTC](https://forum.snapmaker.com/t/partial-blocks-with-wood-pla-filament/32998/1 "2023-09-23T16:54:57Z")

</div>

I seem to be getting regular partial nozzle blocks using the wood PLA filament. The first few items I printed with it were absolutely fine, but I’m currently doing a run of multiple parts and have had a couple of blockages. Now, even after trying to clean the nozzle as best as I can, the parts start fine, but by the end it looks like the nozzle is partially blocked and under extruding quite a lot. They’re not massive parts, only about a 5 hour print.

After the first bigger block, I switched to a new nozzle, so there’s no different type of filament that could be causing issues.

Is this a known problem with the wood filament? Is it worth trying a cleaning filament? I’ve never felt the need for one before now.

---

<div class="post-metadata">

**Author:** ![sdj544](https://sea2.discourse-cdn.com/flex022/user_avatar/forum.snapmaker.com/sdj544/32/11365_2.png) [@sdj544](https://forum.snapmaker.com/u/sdj544)\
**Post date:** [September 23, 2023, 10:28pm UTC](https://forum.snapmaker.com/t/partial-blocks-with-wood-pla-filament/32998/2 "2023-09-23T22:28:47Z")

</div>

Wood filament is highly abrasive. So a lot of problems are solved by using a hardened nozzle. But that’s not usually a clogging issue. It does tend to clog more than normal filament.  
You might want to try increasing temperature.  
Also a lot of people like to use a .6mm nozzle but still with settings for .4mm. Might have to play with flow to get results you need.

-S

---

<div class="post-metadata">

**Author:** ![davidE1A](https://avatars.discourse-cdn.com/v4/letter/d/b19c9b/32.png) [@davidE1A](https://forum.snapmaker.com/u/davidE1A)\
**Post date:** [September 23, 2023, 10:49pm UTC](https://forum.snapmaker.com/t/partial-blocks-with-wood-pla-filament/32998/3 "2023-09-23T22:49:39Z")

</div>

I did just try one with an extra 5 degrees nozzle temp. That one blocked completely!

I have just got some new nozzles, including some 0.6mm ones to try.When you say use a 0.6 but with 0.4mm settings, do you mean literally just change the nozzle and nothing else, or tell cura it’s got a 0.6mm nozzle, but only print with a 0.4mm line width?

---

<div class="post-metadata">

**Author:** ![sdj544](https://sea2.discourse-cdn.com/flex022/user_avatar/forum.snapmaker.com/sdj544/32/11365_2.png) [@sdj544](https://forum.snapmaker.com/u/sdj544)\
**Post date:** [September 24, 2023, 5:47am UTC](https://forum.snapmaker.com/t/partial-blocks-with-wood-pla-filament/32998/4 "2023-09-24T05:47:02Z")

</div>

> [@davidE1A](#):
>
> I did just try one with an extra 5 degrees nozzle temp. That one blocked completely!

Try lowering temp? I’ve heard of some materials getting too hot and basically burning and that causing clogging.

> [@davidE1A](#):
>
> do you mean literally just change the nozzle and nothing else, or tell cura it’s got a 0.6mm nozzle, but only print with a 0.4mm line width?

Just change the nozzle. No change to the settings. Print same as you would with a .4. The idea is that the wood filaments don’t flow quite as freely and having the slightly larger nozzle makes up for that.

(BTW, I haven’t done it personally, but I think it’s been discussed on this forum a few times. Probably a year or two ago. Try a search)

-S

---

<div class="post-metadata">

**Author:** ![sdj544](https://sea2.discourse-cdn.com/flex022/user_avatar/forum.snapmaker.com/sdj544/32/11365_2.png) [@sdj544](https://forum.snapmaker.com/u/sdj544)\
**Post date:** [September 26, 2023, 6:20am UTC](https://forum.snapmaker.com/t/partial-blocks-with-wood-pla-filament/32998/5 "2023-09-26T06:20:37Z")

</div>

One thing I forgot to mention.  
Have you tried drying the filament?  
Wood filament can be especially susceptible to absorbing moisture.

-S

---

<div class="post-metadata">

**Author:** ![davidE1A](https://avatars.discourse-cdn.com/v4/letter/d/b19c9b/32.png) [@davidE1A](https://forum.snapmaker.com/u/davidE1A)\
**Post date:** [September 26, 2023, 11:43am UTC](https://forum.snapmaker.com/t/partial-blocks-with-wood-pla-filament/32998/6 "2023-09-26T11:43:05Z")

</div>

I haven’t, no. But I’m fairly sure I have no other signs of moisture - no popping, blobs or anything. It prints fine, just the line width gets thinner.

But, I am now thinking it might just be that the nozzle has worn out already (especially if the wood filament is that harsh). I had to pause the wood pieces to print a couple of things with normal pla, so I put a new nozzle in, and the first print going back to the wood is looking ok again. Also, I read somewhere that when extruding the filament (when loading), if it curls up coming out the nozzle (which mine was after trying to clean it) then that’s a sign of a worn nozzle.

Part on the left was an early print. The middle, the last complete print it managed, which was after doing about 15 of these. On the right, with a new nozzle again.

 ![IMG_20230926_123411](https://us1.discourse-cdn.com/flex022/uploads/snapmaker/original/3X/c/9/c92e8e2196c0e463c5264b2a1c86ee0f76b92f58.jpeg)

The few tiny gaps I can live with, so I think I’ll see how long this nozzle lasts (I have 50 of these to print!) and then try the 0.6mm if it wears out quickly again.